Crazing

 

 

Description

Appears to the naked eye as a loss of gloss, close examination under low magnification reveals a large number of minute cracks.

Cause

Excessive stresses in the paint film due to:

  1. Inadequate mixing of materials prior to application, insufficient thinning or the wrong grade of thinner.
  2. Excessive film thickness, colour coat applied over inadequately dry or excessively thick under coats.
  3. Incorrect use of additives.

 

Prevention

  1. Always mix paint thoroughly, and use the correct amount of recommended thinner.
  2. Use correct spraying techniques. Apply paint in thin, web films and allow adequate drying time between coats.
  3. Only use approved additives.

 

Rectification

Sand the affected area down to a sound, smooth finish and repaint.

 

 

Other Defects:

Back

Site Cookies

At this PPG site we use essential cookies which are strictly necessary to make this website function properly. We would like to also use some first party and third party optional cookies in order to improve your experience. You can change your cookies settings at any time. For more information read our cookie policy.