Pickling

 

 

Description

Swelling or wrinkling of the paint surface, varying in severity and most often occurring around feathered edges. The underlying paint may break through the topcoat.

Cause

Reaction with the underlying surface resulting from the application of nitro or thermosetting enamels over thermoplastic acrylics or airdrying synthetics.

 

Prevention

Ensure compatibility of materials or that the underlying layer is thoroughly sealed.

 

Rectification

Rub down the affected area, taking care not to uncover any areas which could give rise to the same problem, seal the surface and repaint. In severe cases rub down the affected area to the substrate and repaint.

 

 

Other Defects:

Back

Site Cookies

At this PPG site we use essential cookies which are strictly necessary to make this website function properly. We would like to also use some first party and third party optional cookies in order to improve your experience. You can change your cookies settings at any time. For more information read our cookie policy.